loads of tigs have diffrent settings and knobs understanding what thay do realy helps id be using a 2.4mm tungsen very pointed, 1.6 filler, around 50amps dc and 25 crator/base if you have it, pulse off if you have it, hf start on if you have it 1 sec pre gas 2 sec post gas keep the torch travel constent with around 1.5 mm gap and dip/drag the filler onto the edge of the shiny pool to cool it keeping the bead uniform in with as the work pice heats up you just go a bit quicker not as easy as it sounds ![]() a steady hand makes light work in the tig world i realy miss tig welding Last edited by baz-r : 16th June 2010 at 05:51 PM. |